2.6 Stabilizers
Stabilizers are the lifeline of PVC processing. They deal with two weaknesses of PVC itself: poor thermal stability and aging. A PVC coated fabric formula uses three groups of stabilizers.
| Stabilizer | What It Does | Common Types and Dosage |
|---|---|---|
| Heat Stabilizers | PVC decomposes easily at processing temperatures. Heat stabilizers prevent it from degrading under heat during processing and in use | Lead salts, metal soaps and organotins; usually 2–8 PHR |
| Antioxidants | Delay or inhibit oxidative aging of PVC during processing and in use, extending the life of the fabric | Hindered phenols and phosphites |
| Light Stabilizers / UV Absorbers | Protect the PVC molecular chain from UV damage, so the fabric does not turn brittle, discolor or lose strength in sunlight | Benzophenones; usually 0.3–1 PHR |
2.6.1 Heat Stabilizers and Antioxidants
PVC starts to break down at the temperatures used for calendering, coating and lamination, and the same weakness continues once the fabric is in service. Heat stabilizers are the core protection against this. The common systems are lead salts, metal soaps and organotins, usually added at 2–8 PHR, or parts per hundred parts of PVC resin.
The stabilizer system also has a regulatory side. In the EU, for example, REACH restricts lead in PVC articles to below 0.1% from November 29, 2024. If your fabric is going to the EU or another market with lead limits, tell us at the inquiry stage so the stabilizer system is selected to match.
Antioxidants such as hindered phenols and phosphites work alongside heat stabilizers. They delay or inhibit oxidative aging during processing and in use, which extends the service life of the fabric.
2.6.2 UV Absorbers
Light stabilizers, or UV absorbers, protect the PVC molecular chain from ultraviolet damage. Without them, a fabric left in the sun turns brittle, changes color and loses strength, which is the real answer to whether vinyl fabric fades in the sun. Benzophenone types are the most common, usually at 0.3–1 PHR.
UV protection is almost standard for outdoor PVC tarpaulin, but because of cost pressure in the market, it is not added by default. When a buyer asks for it, UV-531 is the common choice. For longer outdoor life, the absorber can be upgraded:
| Comparison | UV-531 | UV-329 | UV-1164 |
|---|---|---|---|
| Chemical Class | Benzophenone | Benzotriazole | Hydroxyphenyl triazine (HPT) |
| UV Absorption Range | 240–340 nm | 270–400 nm | 260–400 nm, covering the full UV-A and UV-B range |
| Absorption Strength | ★★★☆☆ | ★★★★☆ | ★★★★★ (strongest) |
| Thermal Stability | ★★★☆☆ (good) | ★★★★☆ (excellent) | ★★★★★ (outstanding; 10% weight-loss temperature of 347 °C) |
| Compatibility and Migration | Good compatibility; slightly weaker long-term migration resistance | Excellent compatibility, low migration | Excellent compatibility; resists extraction and volatilization for long-lasting protection |
| Metal Ion Sensitivity | Not sensitive | Not sensitive | Least affected by metal ions, for higher stability |
| Best Suited To | Short-term use or mid- to low-end products | General use, especially clear and light-colored products | Premium, long-life products in harsh outdoor conditions |
| Rating in PVC | Suitable for standard PVC; recommended for short-term or general outdoor use | Suitable for rigid and flexible PVC; recommended for general use | Suitable for PVC; first choice for premium or harsh outdoor use |
| Cost | Low | Medium to high | High |
The choice follows the product. A short-life cover can use UV-531; benzotriazole types such as UV-329 suit clear vinyl fabric and light colors; a triazine such as UV-1164 is reserved for premium products that must last in harsh outdoor conditions. The same logic applies when we formulate UV-resistant PVC tarpaulin for different climates.
If your fabric will be used outdoors, send us the climate, expected service life and color, and we will select the stabilizer and UV package before sampling.